Heat Deflection Temperature under 1.8 MPa Load1
Polymer / HDT (at 1.82 MPa / 264 psi) |
Neat |
30% GF |
Acrylonitrile-butadiene-styrene (ABS) |
94 |
99 |
High Density Polyethylene (HDPE) |
46 |
|
Polyacetal (POM) |
106 |
159 |
Polyamideimide (PAI) |
278 |
281 |
Polybenzimidazole (PBI) |
425 |
|
Polybutylene terephthalate (PBT) |
56 |
209 |
Polycarbonate (PC) |
124 |
142 |
Polycaprolactam (PA6, Nylon 6) |
64 |
207 |
Polyetheretherketone (PEEK) |
159 |
315 |
Polyetherimides (PEI) |
199 |
209 |
Polyetherketone (PEK) |
169 |
319 |
Polyether sulfone (PES,
PSU) |
206 |
211 |
Polyethylene terephthalate (PET) |
71 |
219 |
Polyhexamethylene adipamide (PA66, Nylon 6,6) |
74 |
253 |
Polyimide (PI) |
319 |
|
Polymethyl methacrylate (PMMA) |
83 |
|
Polyphenylene ether (PPE, PPO) |
114 |
139 |
Polyphenylene sulfide (PPS) |
120 |
268 |
Polyphthalamides (PPA) |
127 |
243 |
Polyphenylsulfone (PPSU) |
206 |
215 |
Polypropylene (PP) |
62 |
142 |
Polystyrene (PS) |
79 |
|
|
|
|